Iintonga zeWelding AWS A5.1 E6013 (J421)

Inkcazelo emfutshane:

Iintonga zokuwelda i-AWS A5.1 E6013 (J421) ilungele ukuwelda kwesakhiwo sentsimbi yekhabhoni ephantsi, ngakumbi ukuwelda kwentsimbi yentsimbi ebhityileyo kunye ne-weld emfutshane enesaphulelo kunye nemfuno yokupasa okugudileyo.


Iinkcukacha zeMveliso

Iithegi zeMveliso

Iintonga zokuwelda i-AWS A5.1 E6013 (J421) ilungele ukuwelda kwesakhiwo sentsimbi yekhabhoni ephantsi, ngakumbi ukuwelda kwentsimbi yentsimbi ebhityileyo kunye ne-weld emfutshane enesaphulelo kunye nemfuno yokupasa okugudileyo.

Ukuhlelwa:

ISO 2560-A-E35 0 RA 12

AWS A5.1: E6013

GB/T 5117 E4313

Iimpawu:

I-AWS A5.1 E6013 (J421) luhlobo lwe-electrode ye-rutile.Ngaba i-welding zombini i-AC & DC yomthombo wamandla kwaye inokuba yeyonke indawo.Inomsebenzi obalaseleyo we-welding njenge-arc ezinzileyo, i-spatter encinci, ukususwa kwe-slag lula kunye nokulawula amandla njl njl. I-rutile-cellulosic electrode enobuchule obuhle be-weld kuzo zonke izikhundla ezibandakanya nkqo phantsi.Okugqwesileyo kwe-gap-bridging kunye nesakhono sokubetha i-arc.Kuba ukuwelda tack kunye nomthwalo fit ups.Injongo ngokubanzi kushishino kunye norhwebo, indibano kunye nevenkile welding.

Ingqalelo:

Ngokuqhelekileyo, akufuneki ukuba womise kwakhona i-electrode ngaphambi kokuba udibanise.Xa ichaphazeleka kukufuma, kufuneka yomiswe kwakhona kwi-150℃-170℃ ngeyure eyi-0.5-1.

Indawo yeWelding:

PA, PB, PC, PD, PE, PF

I-AWS A5.1 E6013 ifanelekile kwizakhiwo zokuwelda ezenziwe ngentsimbi ephantsi yekhabhoni, iqhuba kakuhle kakhulu kwi-welding ebhityileyo kunye neepleyiti zentsimbi ezinobungakanani obuncinci kwaye inokusebenza kakuhle kakhulu kwimeko efuna inkangeleko entle necocekileyo.

Ukudityaniswa kwemichiza kuyo yonke iWeld Metal: (%)

Ukuqulunqwa kwemichiza

C

Mn

Si

S

P

Ni

Cr

Mo

V

Iimfuno

≤0.10

0.32-0.55

≤0.30

≤0.030

≤0.035

≤0.30

≤0.20

≤0.30

≤0.08

Iziphumo eziqhelekileyo

0.08

0.37

0.18

0.020

0.025

0.030

0.035

0.005

0.004

IiPropati zeMechanical zeMetal eDiphozithiweyo

Into yovavanyo

Rm (N/mm2)

I-Rel (N/mm2)

A (%)

KV2(J) 0℃

Iimfuno

440-560

≥355

≥22

≥47

Iziphumo eziqhelekileyo

500

430

27

80

Isalathiso sangoku (DC)

Ububanzi

φ2.0

φ2.5

φ3.2

φ4.0

φ5.0

Amperage

40 ~ 70

50 ~ 90

80 ~ 130

150 ~ 210

180 ~ 240

Ukuhlolwa kwe-X-Ray yeRadiographic: